Science and technology

Base Material Matching for Press-In Fasteners: Stainless, Aluminium and Galvanised Sheet

Base Material Matching for Press-In Fasteners: Stainless, Aluminium and Galvanised Sheet

A press-in fastener catalogue usually quotes a sheet thickness range, as if any sheet inside that range would work. On the floor, the same part pressed into cold-rolled steel, stainless and aluminium of equal thickness can differ thirty percent in push-out, and sometimes will not press at all or cracks the sheet. Press-in joining is plastic forming, so success depends on ductility, hardness, work-hardening tendency and surface condition. We meet these issues constantly in selection.

How press-in forming works

The punch drives the knurl or shoulder into the sheet, the material flows plastically under local pressure and fills the serration spaces, and a mechanical interlock remains. Strength depends on three things: how completely the material fills, the contact area between serrations and sheet, and residual compressive stress after pressing. Ductile material fills well and gives high strength; hard material springs back, fills poorly and gives less. One part therefore needs different force and depth on different sheets.

Why stainless is difficult

Stainless work-hardens strongly, so local deformation raises hardness during pressing and makes further flow difficult, leaving shallow insertion and partly unfilled serrations. Springback is also high, so the sheet partly recovers when the punch lifts and the interlock weakens. More force helps, but excessive force cracks the back of thin sheet. Workable measures include stainless-specific parts with sharper serrations and gentler transitions, slightly larger holes, two-stage pressing and controlled punch descent speed.

Aluminium: deformation and collapse

Aluminium is soft and ductile, so pressing is easy - too easy. A little extra depth bulges or even punches through the back, and material is pushed away around the point, leaving a depression that spoils flatness and appearance. Alloys differ widely as well: pure aluminium and low-strength alloys are very soft while hard and high-magnesium grades are clearly stiffer, so they need separate treatment. Aluminium also forms a galvanic couple with stainless or zinc, corroding as the anode.

Coating damage on galvanised sheet

Under the pressure and friction of pressing, zinc coating cracks and flakes, exposing steel that becomes a corrosion origin. White rust appears around the press point and later turns red. Controls include parts with a sealing shoulder, reduced insertion depth, touch-up with zinc-rich paint or protective oil after pressing, and avoiding a bend close to the press point, which worsens coating damage. On coastal or outdoor projects the press point is usually where the part rusts first.

Pre-coated and special surfaces

Pre-coated sheet has a more brittle coating than zinc and cracks under pressing, leaving a corrosion path and a visible defect. Use dedicated punches with flatter faces and larger edge radii, keep insertion to the minimum, and add a cap or gasket over the point. Brushed and mirror stainless also need protection against punch scratches, usually a protective film or a soft-faced punch. For these appearance parts the defect is scratching rather than strength, so the control focus shifts.

Reading hardness together with thickness

Thickness alone is not a selection basis; read it with hardness. The same part presses normally in 1.5 mm cold-rolled steel, may not press at all in 1.5 mm stainless, and may punch through 1.5 mm aluminium. A two-dimensional table works well: thickness on one axis, hardness or grade on the other, with the recommended part and force range in each cell. That is far more useful than a single thickness range and gives the shop a basis for setting up.

Hole size and tolerance

Press-in parts specify a hole size, typically with a tolerance of a few hundredths of a millimetre. Too small and resistance rises until the part bends or the sheet cracks; too large and the material cannot fill the serrations, so push-out falls. Hole quality matters as much: a punched edge with burr or taper tilts the part. Check punch wear periodically in volume production, because wear enlarges the hole gradually and drops strength across the board.

Strength differences and a selection checklist

Push-out strength for one part size falls progressively from cold-rolled steel to galvanised, stainless and aluminium, so design values must come from measured data on the actual sheet with margin, not from the catalogue figure. A checklist should cover base grade and hardness, thickness and tolerance, hole size and punching method, part type and serration form, force and insertion depth, plus corrosion and appearance requirements. We run press trials on the customer's sheet to confirm selection.

CONTACT US

Contact: Mr. Deng

Phone: 13928071304

Tel: 0756-8586520

Email: lizhong@zhjiali.com

Add: 102, Building 4, No. 4 Fuyuan Road, Waisha Village, Shenwan Town, Zhongshan City, Guangdong Province,China